(K.6Na.4)Cl Walker D, Verma P K, Cranswick L M D, Jones R L, Clark S M, Buhre S American Mineralogist 89 (2004) 204-210 Halite-sylvite thermoelasticity Sample: als13k60, T = 500 C, P = 0.0 kbar, cell volume = 237.83 ang**3 _database_code_amcsd 0003277 CELL PARAMETERS: 6.1957 6.1957 6.1957 90.000 90.000 90.000 SPACE GROUP: Fm3m X-RAY WAVELENGTH: 1.541838 Cell Volume: 237.832 Density (g/cm3): 1.902 MAX. ABS. INTENSITY / VOLUME**2: 30.96824674 RIR: 5.302 RIR based on corundum from Acta Crystallographica A38 (1982) 733-739 2-THETA INTENSITY D-SPACING H K L Multiplicity 28.82 100.00 3.0979 2 0 0 6 41.21 63.49 2.1905 2 2 0 12 51.07 19.50 1.7885 2 2 2 8 59.70 8.07 1.5489 4 0 0 6 67.62 20.07 1.3854 4 2 0 24 75.12 13.65 1.2647 4 2 2 24 89.48 3.95 1.0953 4 4 0 12 ================================================================================ XPOW Copyright 1993 Bob Downs, Ranjini Swaminathan and Kurt Bartelmehs For reference, see Downs et al. (1993) American Mineralogist 78, 1104-1107.