Almandine
      Heritsch H
      Zeitschrift fur Kristallographie 85 (1933) 392-403
      Roentgenographische Untersuchungen an einem Granat aus der
      Lieserschlucht bei Spittal a. d. Drau (Kaernten)
      _cod_database_code 1010999
      _database_code_amcsd 0017914

      CELL PARAMETERS:   11.6680  11.6680  11.6680   90.000   90.000   90.000
      SPACE GROUP: Ia3d      
      X-RAY WAVELENGTH:     1.541838
      Cell Volume:   1588.508
      Density (g/cm3):      4.026
      MAX. ABS. INTENSITY / VOLUME**2:      32.26127080    
      RIR:      2.609
      RIR based on corundum from Acta Crystallographica A38 (1982) 733-739
               2-THETA      INTENSITY    D-SPACING   H   K   L   Multiplicity
                18.63          1.01        4.7634    2   1   1        24
                28.63          2.07        3.1184    3   2   1        48
                30.65         32.35        2.9170    4   0   0         6
                34.37        100.00        2.6090    4   2   0        24
                36.11          4.34        2.4876    3   3   2        24
                37.77         26.51        2.3817    4   2   2        24
                39.38         11.61        2.2883    4   3   1        48
                42.43         13.93        2.1303    5   2   1        48
                43.89          2.02        2.0626    4   4   0        12
                48.07         10.53        1.8928    6   1   1        24
                48.07         10.86        1.8928    5   3   2        48
                54.48         12.20        1.6841    4   4   4         8
                56.91         24.73        1.6181    6   4   0        24
                59.26         39.70        1.5592    6   4   2        48
                63.82          8.27        1.4585    8   0   0         6
                72.45          8.80        1.3045    8   4   0        24
                74.54         15.26        1.2731    8   4   2        48
                76.60          5.70        1.2438    6   6   4        24
                81.70          1.22        1.1786    9   4   1        48
                81.70          1.04        1.1786    8   5   3        48
                84.72          1.14        1.1441   10   2   0        24
================================================================================
       XPOW Copyright 1993 Bob Downs, Ranjini Swaminathan and Kurt Bartelmehs
  For reference, see Downs et al. (1993) American Mineralogist 78, 1104-1107.