Bismuth
      Straumanis M E
      Journal of Applied Physics 20 (1949) 726-734
      The precision determination of lattice constants by the powder and rotation
      crystal methods and applications
      Locality: synthetic
      Sample: at T = 25 C
      _database_code_amcsd 0012876

      CELL PARAMETERS:    4.5367   4.5367   5.1998   90.000   90.000  120.000
      SPACE GROUP: P6_3/mmc  
      X-RAY WAVELENGTH:     1.541838
      Cell Volume:     92.685
      Density (g/cm3):      7.487
      MAX. ABS. INTENSITY / VOLUME**2:      635.0862849    
      RIR:     27.620
      RIR based on corundum from Acta Crystallographica A38 (1982) 733-739
               2-THETA      INTENSITY    D-SPACING   H   K   L   Multiplicity
                22.63         29.90        3.9289    1   0   0         6
                28.47        100.00        3.1347    1   0   1        12
                34.50         13.15        2.5999    0   0   2         2
                39.74         26.14        2.2684    1   1   0         6
                41.66         11.33        2.1682    1   0   2        12
                46.21          4.10        1.9645    2   0   0         6
                49.61         19.55        1.8377    2   0   1        12
                53.62         20.12        1.7093    1   1   2        12
                58.17         11.41        1.5858    1   0   3        12
                58.93          3.64        1.5674    2   0   2        12
                62.55          2.95        1.4850    2   1   0        12
                65.35         15.16        1.4279    2   1   1        24
                72.12          3.58        1.3096    3   0   0         6
                72.75          1.16        1.3000    0   0   4         2
                72.76          5.20        1.2997    2   0   3        12
                73.43          3.36        1.2895    2   1   2        24
                77.31          1.41        1.2342    1   0   4        12
                82.46          4.59        1.1696    3   0   2        12
                86.24          4.02        1.1279    1   1   4        12
                86.25          6.02        1.1277    2   1   3        24
================================================================================
       XPOW Copyright 1993 Bob Downs, Ranjini Swaminathan and Kurt Bartelmehs