Megawite Zhao J, Ross N L, Angel R J Physics and Chemistry of Minerals 31 (2004) 299-305 Tilting and distortion of CaSnO3 perovskite to 7 GPa determined from single-crystal X-ray diffraction Note: P = 1.50 GPa Locality: synthetic _database_code_amcsd 0018607 5.4952 5.6486 7.8561 90 90 90 Pbnm atom x y z Biso B(1,1) B(2,2) B(3,3) B(1,2) B(1,3) B(2,3) Ca -.01276 .0509 .25 .556 .0046 .0042 .00235 .00002 0 0 Sn 0 .5 .5 .305 .00242 .00285 .00105 -.00001 -.00002 .00010 O1 .1009 .4637 .25 .63 .0062 .0062 .0014 .0010 0 0 O2 .6970 .2995 .0514 .59 .0010 .0062 .0035 -.0016 .0007 -.0006